Skip to content

A2 Tool Steel

1.2363

  • EN1.2363
  • ENX100CrMoV5
  • AISIA2

Air-hardening cold work steel (AISI A2) with 1 % carbon and 5 % chromium. It distorts little in heat treatment and at 58–62 HRC balances wear resistance against toughness; used for blanking dies, punches and gauges that need more toughness than 1.2379.

Spectral Analysis

wt. % · EN ISO 4957 ranges
C
0.95–1.05
Si
0.10–0.40
Mn
0.40–0.80
Cr
4.80–5.50
Mo
0.90–1.20
V
0.15–0.35

Typical ranges according to the standard, for information only. The analysis on the material certificate applies on delivery.

01Material Properties

  • Air hardening; low distortion
  • Balance of wear resistance and toughness
  • Good dimensional stability
  • Good machinability and grindability
  • Can be PVD coated
  • Heat treated to 58–62 HRC

02Applications

  • Blanking and punching dies, punches
  • Shear and cutting blades
  • Thread rolling and cold forming tools
  • Mold components for abrasive plastics
  • Gauges and measuring tools

03Delivery Condition

  • Max. 241 HB, soft annealed.

04Heat Treatment

Heat Treatment Steps

Stress relievingTemperatureTime →600–650 °C
HardeningTemperatureTime →Preheat~650 °CAustenitise940–980 °C

Quench: Air/pressurised gas or 500–550 °C salt bath

TemperingTemperatureTime →1. temper150–250 °C2. temper150–250 °C
Stages and temperatures are typical values; soaking times depend on section size.

Tempering Diagram

0 °C → 64 HRC100 °C → 63 HRC200 °C → 61.5 HRC300 °C → 59.5 HRC400 °C → 58 HRC500 °C → 58.5 HRC525 °C → 59 HRC550 °C → 57 HRC600 °C → 52 HRC0100200300400500600455055606570Tempering temperature [°C]Hardness [HRC]1.2363Heat treatment: 940–980 °CQuench: Air/pressurisedgas or 500–550 °C salt ba…
Approximate hardness versus tempering temperature after hardening from the typical austenitising temperature.

Values are approximate and for information only; they vary with section size, heat and furnace conditions. Binding values are determined from the manufacturer’s data under laboratory conditions.

05Mechanical Properties

Typical values by delivery and heat-treatment condition; actual values depend on section size and heat-treatment parameters.

ConditionHardnessTensile strength Rm (MPa)Note
Soft annealed (delivery)Max. 241 HB≈ 820 (max.)Machinable condition
Hardened (940–980 °C)≈ 62–64 HRC—Before tempering
Low-temperature tempering (150–250 °C)60–62 HRC—Balance of wear resistance and toughness
High-temperature tempering (500–550 °C)58–60 HRC—Secondary hardening; when PVD coating is planned

Typical values; at high hardness, hardness rather than tensile strength is used, and the annealed Rm value is an approximate conversion from hardness. The applicable specification and material certificate govern for orders.

06Applicable Standards & Specifications

  • EN ISO 4957 — Tool steels (X100CrMoV5)
  • ASTM A681 — Alloy tool steels (A2)
  • JIS G4404 — Alloy tool steels (SKD12; similar composition, not identical)
  • DIN 17350 (withdrawn, still used as a reference)

A product specification and an inspection document are different things: e.g. AMS 4928 is a product specification, EN 10204 3.1 is a type of inspection document; one does not replace the other.

07Microstructure & Metallurgical Properties

Typical microstructure information

1.2363 (A2) is an air-hardening cold-work tool steel with 1 % carbon and 5 % chromium. Depending on the heat treatment condition, its microstructure typically consists of a martensitic matrix with dispersed alloy carbides.

Typical metallurgical characteristics

  • Dispersed alloy carbides in a martensitic matrix
  • Smaller and fewer carbides than ledeburitic grades
  • Balance of wear resistance and toughness
  • Air hardening with low distortion
  • Properties influenced by hardening and tempering parameters
1.Typical microstructure
In the hardened and tempered condition: tempered martensite, dispersed alloy carbides and, depending on the tempering temperature, some retained austenite. In the soft-annealed delivery condition: spheroidised carbides in a ferritic matrix.
2.Heat treatment influence
The austenitising temperature (940–980 °C) controls carbide dissolution and hardness. Low-temperature tempering retains hardness; tempering at 500–550 °C gives secondary hardening and reduces retained austenite. Annealed and hardened 1.2363 do not show the same microstructure.
3.Grain structure
Prior austenite grain size depends on austenitising temperature and time; excessive temperature can cause grain growth and loss of toughness.
4.Carbide / precipitate distribution
Chromium carbides together with fine carbides containing molybdenum and vanadium. Carbide volume and size are lower than in ledeburitic grades such as 1.2379; distribution depends on section size and forging reduction.
5.Metallographic examination
Batch-specific metallographic examination is available upon request. A microstructure image alone does not prove chemical analysis, mechanical properties or certificate compliance.

Available technical documentation

  • Chemical composition certificate
  • Mechanical test report, where available
  • Heat treatment information, where available
  • Metallographic examination, upon request

Typical microstructure information. Actual microstructure may vary depending on manufacturing route, product form and heat treatment.

08Is there a better material?

Grades in the same material family as A2 with higher wear resistance and higher impact resistance (toughness); up to two suggestions under each heading. Which one fits depends on the application's priority requirement.

Higher wear resistance

Higher impact resistance (toughness)

Suggestions are based on the critical property levels in our grade data; an improvement in one property may require a trade-off in another. The final selection must be made by technical evaluation against operating conditions, heat treatment and specification.

For more information, browse our Technical Insights

09Move Metal Supply Options

Move Metal is not a producer; we source the grade to your specification through our international producer and supplier network. Dimensions, quantity, delivery condition and documentation requirements are reviewed together.

Product forms

  • Round bar
  • Flat bar
  • Plate
  • Block
  • Cut-to-size

Documents and testing

  • EN 10204 3.1 inspection certificate (chemical analysis, delivery hardness)
  • EN 10204 3.2 inspection certificate (on request, third party)
  • Ultrasonic testing (e.g. SEP 1921, EN 10228-3)
  • Microstructure and inclusion rating (e.g. SEP 1614, ASTM E45, EN 10247)
  • Hardness test report (HB / HRC)
Request A2 Quotation

Not sure if A2 is the right material for your application?

Evaluate candidate materials by application, operating conditions and priority properties with the Material Selection Guide.

Find the Right Material

Have a material requirement?

Send us your specification, drawing or RFQ. Our team will review the requirement and identify a suitable supply option.

Request a Quote