Skip to content

1.2360 MOD 8 % Chromium Cold Work Tool Steel

1.2360 MOD

  • EN1.2360
  • ENX48CrMoV8-1-1
  • Ticari8 % Cr soğuk iş çeliği (K340 tipi)

An 8 % chromium cold work steel derived from 1.2360, with carbon raised to 1.05–1.15 % and molybdenum to 2.00–2.30 %. With higher toughness than 1.2379 and coatable thanks to secondary hardening, it is used at 58–62 HRC for thick-sheet blanking and high-volume punch tooling.

Spectral Analysis

wt. % · Tipik analiz ranges
C
1.05–1.15
Si
0.80–1.10
Mn
0.35–0.50
Cr
7.80–8.50
Mo
2.00–2.30
V
0.45–0.55

Typical ranges according to the standard, for information only. The analysis on the material certificate applies on delivery.

01Material Properties

  • Higher toughness than 1.2379
  • Good wear resistance
  • High-temperature tempering (secondary hardening)
  • Low heat-treatment distortion
  • Suitable for PVD / CVD coating and nitriding
  • 58–62 HRC by heat treatment

02Applications

  • Blanking and piercing dies (thick sheet)
  • Deep drawing and forming dies
  • Rolling and clamping tools
  • High-volume punches and dies
  • Powder compaction dies

03Delivery Condition

  • Soft annealed, max. 250 HB.

04Heat Treatment

Heat Treatment Steps

Stress relievingTemperatureTime →600–650 °C
HardeningTemperatureTime →Preheat~800 °CAustenitise1030–1070 °C

Quench: Pressurised gas in vacuum, oil or salt bath 500–550 °C

TemperingTemperatureTime →1. temper500–560 °Cmin. 2 h2. temper500–560 °Cmin. 2 h
Stages and temperatures are typical values; soaking times depend on section size.

Tempering Diagram

0 °C → 63 HRC100 °C → 62 HRC200 °C → 60.5 HRC300 °C → 59 HRC400 °C → 58.5 HRC500 °C → 60 HRC525 °C → 61 HRC550 °C → 60 HRC600 °C → 55 HRC650 °C → 47 HRC010020030040050060070040455055606570Tempering temperature [°C]Hardness [HRC]1.2360 MODHeat treatment: 1030–1070 °CQuench: Pressurised gas invacuum
Approximate hardness versus tempering temperature after hardening from the typical austenitising temperature.

Values are approximate and for information only; they vary with section size, heat and furnace conditions. Binding values are determined from the manufacturer’s data under laboratory conditions.

05Is there a better material?

Grades in the same material family as 1.2360 MOD with higher wear resistance and higher impact resistance (toughness); up to two suggestions under each heading. Which one fits depends on the application's priority requirement.

Higher wear resistance

Higher impact resistance (toughness)

Suggestions are based on the critical property levels in our grade data; an improvement in one property may require a trade-off in another. The final selection must be made by technical evaluation against operating conditions, heat treatment and specification.

For more information, browse our Technical Insights

06Move Metal Supply Options

Move Metal is not a producer; we source the grade to your specification through our international producer and supplier network. Dimensions, quantity, delivery condition and documentation requirements are reviewed together.

Product forms

  • Round bar
  • Flat bar
  • Plate
  • Block
  • Cut-to-size

Documents and testing

  • EN 10204 3.1 inspection certificate (chemical analysis, delivery hardness)
  • EN 10204 3.2 inspection certificate (on request, third party)
  • Ultrasonic testing (e.g. SEP 1921, EN 10228-3)
  • Microstructure and inclusion rating (e.g. SEP 1614, ASTM E45, EN 10247)
  • Hardness test report (HB / HRC)
Request 1.2360 MOD Quotation

Not sure if 1.2360 MOD is the right material for your application?

Evaluate candidate materials by application, operating conditions and priority properties with the Material Selection Guide.

Find the Right Material

Have a material requirement?

Send us your specification, drawing or RFQ. Our team will review the requirement and identify a suitable supply option.

Request a Quote