Alloy 625 (Inconel 625) Nickel Alloy
Alloy 625
Available on Request
- EN2.4856
- ENNiCr22Mo9Nb
- UNSN06625
- TicariInconel® 625
Alloy 625 (2.4856) is a Ni-Cr alloy that gains its strength from the solid-solution effect of Mo and Nb and is not hardenable by heat treatment. Usable from cryogenic temperatures up to 980 °C, it is chosen for marine, chemical and flue-gas equipment and as a welding filler.
Spectral Analysis
wt. % · UNS N06625 ranges- Ni
- ≥58.0
- Cr
- 20.0–23.0
- Mo
- 8.0–10.0
- Nb+Ta
- 3.15–4.15
- Fe
- ≤5.0
- Al
- ≤0.40
- Ti
- ≤0.40
- C
- ≤0.10
Typical ranges according to the standard, for information only. The analysis on the material certificate applies on delivery.

01Material Properties
- High resistance to pitting and crevice corrosion
- Service from cryogenic to 980 °C
- Not hardenable by heat treatment; solid-solution strengthened
- Very good weldability
- High fatigue and thermal fatigue strength
02Applications
- Chemical and petrochemical process equipment
- Marine and offshore components
- Gas turbine exhaust and combustion parts
- Flue gas desulphurisation systems
- Weld overlay and filler
03Delivery Condition
- Annealed (Grade 1) or solution annealed (Grade 2); bar, plate, sheet, tube.
04Heat Treatment
Heat Treatment Steps
Values are approximate and for information only; they vary with section size, heat and furnace conditions. Binding values are determined from the manufacturer’s data under laboratory conditions.
05Mechanical Properties
Values by delivery condition; actual values depend on product form, section size and annealing conditions.
| Condition | Rm (MPa) | Rp0.2 (MPa) | A (%) | Hardness | Basis / note |
|---|---|---|---|---|---|
| Annealed, Grade 1 (bar ≤ 100 mm) | ≥ 827 | ≥ 414 | ≥ 30 | — | ASTM B446 min. |
| Solution annealed, Grade 2 (bar) | ≥ 690 | ≥ 276 | ≥ 30 | — | ASTM B446 min. |
| Annealed, Grade 1 — typical | ≈ 830–1100 | ≈ 415–760 | ≈ 30–60 | ≈ 175–240 HB | Varies with section |
| Solution annealed, Grade 2 — typical | ≈ 720–900 | ≈ 290–415 | ≈ 40–60 | ≈ 115–195 HB | Condition preferred for creep service |
Minimum values apply to the stated standard and condition; typical values (≈) are for guidance. The applicable specification and material certificate govern for orders.
06Applicable Standards & Specifications
- ASTM B443 — Plate, sheet and strip (UNS N06625)
- ASTM B444 — Seamless pipe and tube
- ASTM B446 — Rod and bar
- ASTM B564 — Forgings
- AMS 5666 — Bars, forgings and rings (annealed)
- AMS 5599 — Sheet, strip and plate (annealed)
- NACE MR0175 / ISO 15156 — Sour (H₂S) service (on request)
A product specification and an inspection document are different things: e.g. AMS 4928 is a product specification, EN 10204 3.1 is a type of inspection document; one does not replace the other.
07Microstructure & Metallurgical Properties
Typical microstructure informationAlloy 625 is a solid-solution strengthened Ni-Cr-Mo-Nb alloy. In the delivery condition its microstructure typically consists of a face-centred cubic (FCC) austenitic γ matrix with dispersed primary carbides.
Typical metallurgical characteristics
- FCC austenitic γ matrix (solid-solution strengthened)
- Discrete MC (NbC) and M₆C carbides
- Grain size differs between Grade 1 and Grade 2
- Possible γ'' / δ precipitation on prolonged holding at 600–750 °C
- Properties influenced by annealing condition and service temperature
- 1.Typical microstructure
- In the annealed (Grade 1) or solution-annealed (Grade 2) condition: a single-phase γ matrix with annealing twins and discrete MC (NbC) and M₆C carbides within grains and at grain boundaries.
- 2.Heat treatment influence
- Grade 1 (870–1040 °C) gives a finer-grained, higher-strength structure; Grade 2 (1095–1205 °C) a coarser-grained one, so the two conditions do not show the same microstructure. Prolonged exposure at about 600–750 °C can precipitate γ'' (Ni₃Nb), followed by δ phase and grain-boundary carbides, which raises hardness and lowers ductility.
- 3.Grain structure
- Grain size depends on annealing temperature and prior deformation; the coarser-grained solution-annealed condition is used where creep strength at high temperature is required, the finer-grained annealed condition for room-temperature and fatigue strength.
- 4.Carbide / precipitate distribution
- In the delivery condition mainly NbC-type MC and M₆C carbides. After long-term service or thermal ageing, γ'' and δ (Ni₃Nb) may precipitate; weld metal can show Laves phase associated with Nb segregation.
- 5.Metallographic examination
- Batch-specific metallographic examination is available upon request. A microstructure image alone does not prove chemical analysis, mechanical properties or certificate compliance.
Available technical documentation
- Chemical composition certificate
- Mechanical test report, where available
- Heat treatment information, where available
- Metallographic examination, upon request
Typical microstructure information. Actual microstructure may vary depending on manufacturing route, product form and heat treatment.
08Is there a better material?
Grades in the same material family as Alloy 625 with higher wear resistance and higher impact resistance (toughness); up to two suggestions under each heading. Which one fits depends on the application's priority requirement.
Higher wear resistance
Our list has no grade with higher wear resistance than Alloy 625 without a marked trade-off in its other critical properties.
Higher impact resistance (toughness)
Our list has no grade with higher impact resistance (toughness) than Alloy 625 without a marked trade-off in its other critical properties.
Suggestions are based on the critical property levels in our grade data; an improvement in one property may require a trade-off in another. The final selection must be made by technical evaluation against operating conditions, heat treatment and specification.
For more information, browse our Technical Insights09Move Metal Supply Options
Move Metal is not a producer; we source the grade to your specification through our international producer and supplier network. Dimensions, quantity, delivery condition and documentation requirements are reviewed together.
Product forms
- Round bar
- Plate
- Sheet
- Tube
- Forgings
Documents and testing
- EN 10204 3.1 inspection certificate
- EN 10204 3.2 inspection certificate (upon request, third party)
- Ultrasonic testing (e.g. ASTM E2375), upon request
- Intergranular corrosion testing (e.g. ASTM G28)
- Grain size report (ASTM E112)
Supply status: Available on Request
Request Alloy 625 QuotationNot sure if Alloy 625 is the right material for your application?
Evaluate candidate materials by application, operating conditions and priority properties with the Material Selection Guide.
Find the Right MaterialGrades in the Same Group
Back to GroupTechnical resources for this material
In the glossary
Have a material requirement?
Send us your specification, drawing or RFQ. Our team will review the requirement and identify a suitable supply option.