Skip to content

L6 Hot Work Tool Steel

1.2714

  • EN1.2714
  • EN55NiCrMoV7
  • AISIL6

Ni-Cr-Mo-V alloyed hot work tool steel valued for its toughness under impact and thermal loading. Used for hammer and press forging dies, die holders, and bolsters and backers in aluminium extrusion tooling.

Spectral Analysis

wt. % · EN ISO 4957 ranges
C
0.50–0.60
Si
0.10–0.40
Mn
0.60–0.90
Cr
0.80–1.20
Mo
0.35–0.55
Ni
1.50–1.80
V
0.05–0.15

Typical ranges according to the standard, for information only. The analysis on the material certificate applies on delivery.

01Material Properties

  • Very good toughness
  • Uniform hardness through the core
  • Suitable for surface treatments
  • Available pre-hardened or soft annealed
  • Good hot strength
  • Use above 44 HRC is not recommended

02Applications

  • Hammer forging dies
  • Press forging dies
  • Die holders for press forging
  • Bolsters and backers in aluminium extrusion tooling

03Delivery Condition

  • 230 HB, soft annealed

04Heat Treatment

Heat Treatment Steps

Stress relievingTemperatureTime →550–600 °C
HardeningTemperatureTime →Preheat~625 °CAustenitise840–870 °C

Quench: Oil or 180–220 °C salt bath

TemperingTemperatureTime →1. temper400–600 °C2. temper400–600 °C
Stages and temperatures are typical values; soaking times depend on section size.

Tempering Diagram

0 °C → 57 HRC100 °C → 56 HRC200 °C → 54 HRC300 °C → 51 HRC400 °C → 48 HRC500 °C → 44 HRC550 °C → 40 HRC600 °C → 36 HRC650 °C → 30 HRC0100200300400500600700253035404550556065Tempering temperature [°C]Hardness [HRC]1.2714Heat treatment: 840–870 °CQuench: Oil or 180–220 °Csalt bath
Approximate hardness versus tempering temperature after hardening from the typical austenitising temperature.

Values are approximate and for information only; they vary with section size, heat and furnace conditions. Binding values are determined from the manufacturer’s data under laboratory conditions.

05Mechanical Properties

Typical values by delivery and service condition; actual values depend on section size, cooling rate and heat-treatment parameters.

ConditionHardnessTensile strength Rm (MPa)Note
Soft annealed (delivery)Max. 250 HB≈ 850 (max.)Machinable condition
Pre-hardened (delivery option)36–42 HRC≈ 1150–1300Used without further heat treatment
Hardened (840–870 °C)≈ 56–58 HRC—Before tempering
Hardened + tempered (400–600 °C)36–48 HRC≈ 1150–1600Above 44 HRC not recommended for toughness

Typical values; Rm values are approximate conversions from hardness. The applicable specification and material certificate govern for orders.

06Applicable Standards & Specifications

  • EN ISO 4957 — Tool steels (55NiCrMoV7)
  • ASTM A681 — Alloy tool steels (L6; composition differs from 1.2714)
  • JIS G4404 — Alloy tool steels (SKT4; similar composition, not identical)
  • SEP 1921 — Ultrasonic testing (on request)
  • DIN 17350 (withdrawn, still used as a reference)

A product specification and an inspection document are different things: e.g. AMS 4928 is a product specification, EN 10204 3.1 is a type of inspection document; one does not replace the other.

07Microstructure & Metallurgical Properties

Typical microstructure information

1.2714 is a low-alloy nickel-chromium-molybdenum-vanadium hot-work tool steel. Depending on the heat treatment condition, its microstructure typically consists of a tempered martensitic matrix with fine carbides.

Typical metallurgical characteristics

  • Tempered martensitic matrix; partly bainitic in large sections
  • Low carbide volume; nickel in solid solution
  • Toughness under impact loading
  • Uniform hardenability through the section
  • Properties influenced by hardening and tempering parameters
1.Typical microstructure
In the hardened and tempered (or pre-hardened) condition: tempered martensite with finely dispersed carbides; in large sections the bainite fraction in the core may increase. In the soft-annealed delivery condition: spheroidised carbides in a ferritic matrix.
2.Heat treatment influence
Austenitising takes place at a relatively low 840–870 °C; cooling rate and section size determine the martensite/bainite ratio, and the tempering temperature sets the balance between hardness and toughness. Annealed, pre-hardened and hardened-and-tempered 1.2714 do not show the same microstructure.
3.Grain structure
Prior austenite grain size depends on austenitising temperature and time; the vanadium addition helps restrict grain growth, while excessive temperature can cause grain growth and loss of toughness.
4.Carbide / precipitate distribution
Fine cementite formed during tempering, together with alloy carbides containing chromium, molybdenum and vanadium. Carbide volume is lower than in high-alloy hot work steels; nickel does not form carbides and stays in solution in the matrix.
5.Metallographic examination
Batch-specific metallographic examination is available upon request. A microstructure image alone does not prove chemical analysis, mechanical properties or certificate compliance.

Available technical documentation

  • Chemical composition certificate
  • Mechanical test report, where available
  • Heat treatment information, where available
  • Metallographic examination, upon request

Typical microstructure information. Actual microstructure may vary depending on manufacturing route, product form and heat treatment.

08Is there a better material?

Grades in the same material family as L6 with higher wear resistance and higher impact resistance (toughness); up to two suggestions under each heading. Which one fits depends on the application's priority requirement.

Higher wear resistance

Higher impact resistance (toughness)

Our list has no grade with higher impact resistance (toughness) than L6 without a marked trade-off in its other critical properties.

Suggestions are based on the critical property levels in our grade data; an improvement in one property may require a trade-off in another. The final selection must be made by technical evaluation against operating conditions, heat treatment and specification.

For more information, browse our Technical Insights

09Move Metal Supply Options

Move Metal is not a producer; we source the grade to your specification through our international producer and supplier network. Dimensions, quantity, delivery condition and documentation requirements are reviewed together.

Product forms

  • Round bar
  • Flat bar
  • Plate
  • Block
  • Cut-to-size

Documents and testing

  • EN 10204 3.1 inspection certificate (chemical analysis, delivery hardness)
  • EN 10204 3.2 inspection certificate (on request, third party)
  • Ultrasonic testing (e.g. SEP 1921, EN 10228-3)
  • Microstructure and inclusion rating (e.g. SEP 1614, ASTM E45, EN 10247)
  • Hardness test report (HB / HRC)
Request L6 Quotation

Not sure if L6 is the right material for your application?

Evaluate candidate materials by application, operating conditions and priority properties with the Material Selection Guide.

Find the Right Material

Technical resources for this material

In the glossary

Have a material requirement?

Send us your specification, drawing or RFQ. Our team will review the requirement and identify a suitable supply option.

Request a Quote