15-5 PH Stainless Steel

1.4545 (15-5 PH)

  • EN1.4545
  • ENX5CrNiCu15-5
  • UNSS15500
  • Ticari15-5 PH

Martensitic precipitation-hardening stainless steel based on chromium, nickel and copper with a niobium addition (UNS S15500). Used for turbine, marine and chemical process parts that need strength together with corrosion resistance; supplied at 35–42 HRC.

Spectral Analysis

wt. % · ASTM A564 (XM-12) ranges
C
≤0.07
Si
≤1.00
Mn
≤1.00
Cr
14.0–15.5
Ni
3.50–5.50
Cu
2.50–4.50
Nb
0.15–0.45

Typical ranges according to the standard, for information only. The analysis on the material certificate applies on delivery.

01Applications

  • Aerospace and energy equipment parts (service temperature limited, typically ≈ 300 °C)
  • Marine, shipbuilding, water treatment plants and oil platforms
  • Chemical industry
  • Petrochemical plants
  • Food industry

02Delivery Condition

  • 35–42 HRC

03Heat Treatment

Heat Treatment Steps

Solution treatmentTemperatureTime →1020–1060 °C
AgeingTemperatureTime →~552 °C
Stages and temperatures are typical values; soaking times depend on section size.

Ageing Diagram

0 °C → 35 HRC482 °C → 43 HRC496 °C → 41 HRC552 °C → 37 HRC580 °C → 35 HRC593 °C → 33 HRC621 °C → 31 HRC650 °C → 28 HRC010020030040050060070020253035404550Ageing temperature [°C]Hardness [HRC]1.4545 (15-5 PH)Solution treatment: 1020–1060 °C
Approximate hardness versus ageing temperature after solution treatment (0 °C = solution-treated condition).

Values are approximate and for information only; they vary with section size, heat and furnace conditions. Binding values are determined from the manufacturer’s data under laboratory conditions.

04Mechanical Properties

Minimum values to ASTM A564 in the aged conditions (bar); the solution-treated (A) condition has a hardness limit only. As the ageing temperature rises, strength decreases while ductility and toughness increase.

ConditionAgeingRm min. (MPa)Rp0.2 min. (MPa)A min. (%)Hardness (HRC)
Solution treated (A)1020–1060 °C, rapid cooling———Max. 38
H900482 °C, 1 h1310117010Min. 40
H925496 °C, 4 h1170107010Min. 38
H1025552 °C, 4 h1070100012Min. 35
H1075580 °C, 4 h100086013Min. 32
H1150621 °C, 4 h93072516Min. 28

Values are ASTM A564 XM-12 minimums; additional requirements (e.g. reduction of area, impact) may apply by section and product form. For AMS orders the values of the relevant specification apply. The applicable specification and material certificate govern for orders.

05Applicable Standards & Specifications

  • ASTM A564 — Hot-rolled and cold-finished age-hardening stainless steel bars (XM-12)
  • ASTM A693 — Precipitation-hardening stainless plate, sheet and strip (XM-12)
  • ASTM A705 — Age-hardening stainless steel forgings (XM-12)
  • AMS 5659 — 15-5 PH, consumable-electrode vacuum remelted (CEVM) bars and forgings (aerospace, on request)
  • AMS 5862 — 15-5 PH sheet, strip and plate (on request)
  • AMS 2759/3 — Heat treatment of precipitation-hardening corrosion-resistant steels

A product specification and an inspection document are different things: e.g. AMS 4928 is a product specification, EN 10204 3.1 is a type of inspection document; one does not replace the other.

06Microstructure & Metallurgical Properties

Typical microstructure information

15-5 PH is a low-carbon martensitic precipitation-hardening stainless steel. In the solution-treated condition it consists of lath martensite; strength is developed by fine copper-rich particles that precipitate during ageing.

Typical metallurgical characteristics

  • Low-carbon lath martensite matrix
  • Structure typically free of delta ferrite
  • Hardening by fine copper-rich precipitates
  • More balanced transverse ductility and toughness
  • Strength–toughness balance set by ageing temperature
1.Typical microstructure
Solution treated (A): lath martensite. Aged conditions: finely dispersed copper-rich precipitates in a martensitic matrix. Owing to its compositional balance, the structure is typically free of delta ferrite.
2.Heat treatment influence
At low ageing temperatures (H900) fine, dense precipitates give the highest strength; towards H1025–H1150 the precipitates coarsen, some reverted austenite may form and toughness increases. Solution-treated and aged 1.4545 do not show the same microstructure.
3.Grain structure
Prior austenite grain size depends on solution treatment temperature and time; martensite forms as packets and laths within these grains. Vacuum remelted (CEVM / ESR) production lowers the inclusion level.
4.Carbide / precipitate distribution
Copper-rich (ε-Cu) precipitates on ageing; niobium carbides (NbC) tie up carbon. Reverted austenite may form at higher ageing temperatures.
5.Metallographic examination
Batch-specific metallographic examination is available upon request. A microstructure image alone does not prove chemical analysis, mechanical properties or certificate compliance.

Available technical documentation

  • Chemical composition certificate
  • Mechanical test report, where available
  • Heat treatment information, where available
  • Metallographic examination, upon request

Typical microstructure information. Actual microstructure may vary depending on manufacturing route, product form and heat treatment.

07Is there a better material?

Grades in the same material family as 15-5 PH with higher wear resistance and higher impact resistance (toughness); up to two suggestions under each heading. Which one fits depends on the application's priority requirement.

Higher wear resistance

Higher impact resistance (toughness)

Suggestions are based on the critical property levels in our grade data; an improvement in one property may require a trade-off in another. The final selection must be made by technical evaluation against operating conditions, heat treatment and specification.

For more information, browse our Technical Insights

08Move Metal Supply Options

Move Metal is not a producer; we source the grade to your specification through our international producer and supplier network. Dimensions, quantity, delivery condition and documentation requirements are reviewed together.

Product forms

  • Round bar
  • Flat bar
  • Plate
  • Sheet
  • Forgings
  • Cut-to-size

Documents and testing

  • EN 10204 3.1 inspection certificate
  • EN 10204 3.2 inspection certificate (upon request, third party)
  • Ultrasonic testing (e.g. EN 10308, ASTM A388), upon request
  • Intergranular corrosion testing (e.g. ASTM A262, EN ISO 3651-2)
  • Detrimental phase testing for duplex steels (ASTM A923)
Request 15-5 PH Quotation

Not sure if 15-5 PH is the right material for your application?

Evaluate candidate materials by application, operating conditions and priority properties with the Material Selection Guide.

Find the Right Material

Have a material requirement?

Send us your specification, drawing or RFQ. Our team will review the requirement and identify a suitable supply option.

Request a Quote