M2 High-Speed Steel
1.3343
- EN1.3343
- ENHS6-5-2C
- AISIM2
Cobalt-free molybdenum-tungsten high speed steel (M2). Its use extends from drills, milling cutters, taps, reamers and circular saws to bolt and nut forming dies and cold extrusion punches.
Spectral Analysis
wt. % · EN ISO 4957 ranges- C
- 0.86–0.94
- Cr
- 3.80–4.50
- Mo
- 4.70–5.20
- V
- 1.70–2.10
- W
- 5.90–6.70
Typical ranges according to the standard, for information only. The analysis on the material certificate applies on delivery.

01Applications
- Milling cutters, taps and reamers
- Twist drills
- Countersinks
- Circular saws
- Broaches
- Slitting cutters
- Wood-machining milling cutters
- Planer knives and other cutting tools
- Dies for cold forming of bolts and nuts
- Punches and expanding tools
- Punches and dies used in cold extrusion
02Delivery Condition
- Max. 269 HB, soft annealed (EN ISO 4957).
03Heat Treatment
Heat Treatment Steps
Quench: 500–550 °C salt bath + air
Tempering Diagram
Values are approximate and for information only; they vary with section size, heat and furnace conditions. Binding values are determined from the manufacturer’s data under laboratory conditions.
04Mechanical Properties
Typical values by delivery and heat-treatment condition; actual values depend on section size and heat-treatment parameters.
| Condition | Hardness | Tensile strength Rm (MPa) | Note |
|---|---|---|---|
| Soft annealed (delivery) | Max. 269 HB (EN ISO 4957) | ≈ 910 (max.) | Machinable condition |
| Hardened (1190–1230 °C) | ≈ 63–65 HRC | — | Before tempering; contains retained austenite |
| Hardened + triple tempered (540–570 °C) | 62–66 HRC | — | Typical service range |
Typical values; at high hardness, hardness rather than tensile strength is used, and the annealed Rm value is an approximate conversion from hardness. The applicable specification and material certificate govern for orders.
05Applicable Standards & Specifications
- EN ISO 4957 — Tool steels (HS6-5-2C)
- ASTM A600 — High-speed tool steels (M2)
- JIS G4403 — High-speed tool steels (SKH51; similar composition, not identical)
- DIN 17350 (withdrawn, still used as a reference)
A product specification and an inspection document are different things: e.g. AMS 4928 is a product specification, EN 10204 3.1 is a type of inspection document; one does not replace the other.
06Microstructure & Metallurgical Properties
Typical microstructure information1.3343 (M2) is a cobalt-free tungsten-molybdenum high-speed steel alloyed with vanadium and chromium. Depending on the heat treatment condition, its microstructure typically consists of a tempered martensitic matrix with dispersed primary and secondary carbides.
Typical metallurgical characteristics
- Tempered martensitic matrix
- Primary MC and M6C carbides
- Secondary hardening on tempering at 540–570 °C
- Hot hardness and wear resistance
- Properties influenced by austenitising and tempering parameters
- 1.Typical microstructure
- In the hardened and triple-tempered condition: tempered martensite, undissolved primary MC and M6C carbides and fine secondary carbides precipitated during tempering. In the soft-annealed delivery condition: spheroidised carbides in a ferritic matrix.
- 2.Heat treatment influence
- The high austenitising temperature (1190–1230 °C) takes part of the carbides into solution; the as-quenched structure contains retained austenite. Repeated tempering at 540–570 °C produces secondary hardening and transforms the retained austenite. Annealed and hardened-and-tempered 1.3343 do not show the same microstructure.
- 3.Grain structure
- Grain size is very sensitive to austenitising temperature and time; undissolved carbides restrict grain growth, while exceeding the upper limit causes grain growth and loss of toughness. In high-speed steels grain size is usually assessed by the Snyder-Graff method.
- 4.Carbide / precipitate distribution
- Tungsten- and molybdenum-rich M6C and vanadium-rich MC carbides; fine secondary carbides precipitate during tempering. Carbide size and distribution depend on the production route (conventional / powder metallurgy), section size and forging reduction; in conventionally produced large sections carbide banding may occur.
- 5.Metallographic examination
- Batch-specific metallographic examination is available upon request. A microstructure image alone does not prove chemical analysis, mechanical properties or certificate compliance.
Available technical documentation
- Chemical composition certificate
- Mechanical test report, where available
- Heat treatment information, where available
- Metallographic examination, upon request
Typical microstructure information. Actual microstructure may vary depending on manufacturing route, product form and heat treatment.
07Is there a better material?
Grades in the same material family as M2 with higher wear resistance and higher impact resistance (toughness); up to two suggestions under each heading. Which one fits depends on the application's priority requirement.
Higher wear resistance
- M42 High-Speed Steel
Wear resistance: High · same level, higher carbide volume / hot hardness (wear ranking 60 → 66)
Trade-off: Toughness
- M3:2 High Speed Steel
Wear resistance: High → Very high
Trade-off: Toughness
Higher impact resistance (toughness)
Our list has no grade with higher impact resistance (toughness) than M2 without a marked trade-off in its other critical properties.
Suggestions are based on the critical property levels in our grade data; an improvement in one property may require a trade-off in another. The final selection must be made by technical evaluation against operating conditions, heat treatment and specification.
For more information, browse our Technical Insights08Move Metal Supply Options
Move Metal is not a producer; we source the grade to your specification through our international producer and supplier network. Dimensions, quantity, delivery condition and documentation requirements are reviewed together.
Product forms
- Round bar
- Flat bar
- Plate
- Cut-to-size
Documents and testing
- EN 10204 3.1 inspection certificate (chemical analysis, delivery hardness)
- EN 10204 3.2 inspection certificate (on request, third party)
- Carbide distribution / microstructure evaluation (e.g. SEP 1615)
- Decarburisation depth check
- Ultrasonic testing, on request
Not sure if M2 is the right material for your application?
Evaluate candidate materials by application, operating conditions and priority properties with the Material Selection Guide.
Find the Right MaterialTechnical resources for this material
Have a material requirement?
Send us your specification, drawing or RFQ. Our team will review the requirement and identify a suitable supply option.